固溶前退火处理对2050铝锂合金冷轧薄板力学性能与组织的影响
CSTR:
作者:
作者单位:

中南大学材料科学与工程学院,长沙 410083

作者简介:

蔡文鑫,1993年出生,硕土研究生,主要研究铝锂合金组织和性能。E-mail:506680229@qq.com

通讯作者:

李劲风,1971年出生,博士,教授,主要从事铝锂合金及其腐蚀与防护研究。E-mail:lijinfeng@csu.edu.cn

中图分类号:

TS912+.3

基金项目:

863项目 2013AA032401;中南大学教师基金 2013JSJJ001863项目(No.2013AA032401);中南大学教师基金(No.2013JSJJ001)


Mechanical Property and Structure Variation of 2050 Al-Li Alloy Sheet Caused by Annealing Prior to Solution Treatment
Author:
Affiliation:

School of Materials Science and Engineering,Central South University,Changsha 410083

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    采用拉伸性能测试、电子背散射衍射分析(EBSD)、扫描电子显微镜(SEM)和透射电子显微镜(TEM),研究了固溶前退火处理(300℃/4 h,400℃/2 h)对2050铝锂合金冷轧薄板T8时效后力学性能、晶粒组织和析出相的影响。研究结果表明: 固溶前退火处理导致2050铝锂合金冷轧薄板固溶态不完全再结晶数量增多,晶粒长厚比增大,小角度晶界比例增加,同时使合金Goss织构密度增大。T8时效后主要强化相为T1相和θ'相。固溶前退火处理可导致后续T8时效时T1相在不同{111}Al面上析出差异,其中部分{111}Al面上T1相析出减少,而预拉伸变形时承受高分切应力{111}Al面上T1相析出增加,从而影响合金的力学性能。固溶前300℃/4 h退火处理可使T8时效后合金屈服强度和抗拉强度提高,伸长率基本保持不变。

    Abstract:

    The mechanical properties, grain structures and precipitates of 2050 Al-Li alloy cold-rolled sheet in T8 temper with different annealing prior to solution treatment were investigated by tensile tests, electron backscattering diffraction analysis (EBSD), scanning lectron microscope (SEM) and transmission electron microscope (TEM). The results show that the number of incomplete recrystallization, the aspect ratio of the grains and the number of the low angle grain boundaries and the fraction of Goss texture increase in 2050 Al-Li alloy cold-rolled sheet with annealing prior to solution treatment. The main strengthening precipitates are T1 and θ' phase. The annealing prior to solution treatment leads to the precipitation differences of T1 phase on different {111}Al surfaces during T8 aging process. T1 phase number on some {111}Al surfaces decreases, while it increases on some {111}Al surfaces with high shear stress during pre-tensile deformation. This therefore changes the mechanical properties of the alloy. The annealing at 300℃ for 4 h prior to solution treatment enhances the yield strength and the tensile strength of the alloy cold-rolled sheet with T8 ageing, but the elongation is kept unchanged.

    参考文献
    相似文献
    引证文献
引用本文

蔡文鑫,李劲风,陆丁丁,刘丹阳,宁红.固溶前退火处理对2050铝锂合金冷轧薄板力学性能与组织的影响[J].宇航材料工艺,2019,49(6):47-52.

复制
分享
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2019-05-13
  • 最后修改日期:
  • 录用日期:
  • 在线发布日期: 2019-12-30
  • 出版日期:
文章二维码